Material Data Center is a leading international information system for the plastics industry. Material Data Center offers a comprehensive plastics database, calculation tools, CAE interfaces, a literature database and an application database. For more information about Material Data Center visit www.materialdatacenter.com.
This is the free Material Data Center Datasheet of Ultramid® B3GM35 Q643 - PA6-(GF+MD)40 - BASF
unit conversion, PDF datasheet print, comparison with other plastics, snap fit calculation, beam deflection calculation, CAE Interfaces
Check here, which other Ultramid B datasheets, application examples or technical articles are available in Material Data Center
Ultramid® B3GM35 Q643 is a combined glass-fiber and mineral reinforced injection molding PA6 grade.
Typical applications include industrial articles requiring medium rigidity and high dimensional stability.
Propriétés mécaniques | sec / cond | Unité | Norme du test | ||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||
ISO Data | |||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||
Module en traction | 8100 / * | MPa | ISO 527 | ||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||
Contrainte à la rupture | 117 / - | MPa | ISO 527 | ||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||
Déformation à la rupture | 2.7 / - | % | ISO 527 | ||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||
Résistance au choc Charpy (entaillé), +23°C | 4.1 / - | kJ/m² | ISO 179/1eA |
Propriétés thermiques | sec / cond | Unité | Norme du test | ||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||
ISO Data | |||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||
Température de fusion, 10°C/min | 220 / * | °C | ISO 11357-1/-3 | ||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||
Température de fléchissement s/chrg, 1.80 MPa | 195 / * | °C | ISO 75-1/-2 |
Propriétés diverses | sec / cond | Unité | Norme du test |
Absorption d'eau | 5.7 / * | % | Sim. to ISO 62 |
Absorption d'humidité | 1.7 / * | % | Sim. to ISO 62 |
Masse volumique | 1480 / - | kg/m³ | ISO 1183 |
Recommandations pour la transformation Moulage par injection | Valeur | Unité | Norme du test |
Pré-séchage - température | 80 | °C | - |
Pré-séchage - temps | 2 - 4 | h | - |
L'humidité de traitement | ≤0.1 | % | - |
Température de la matière fondue | 270 - 295 | °C | - |
Température du moule | 80 - 95 | °C | - |
Product is supplied in sealed containers and drying prior to molding is not required. If drying becomes necessary, a dehumidifying or desiccant dryer operating at 80 degC (176 degF) is recommended. Drying time is dependent on moisture level, but 2-4 hours is generally sufficient.
Further information concerning safe handling procedures can be obtained from the Material Safety Data Sheet. Alternatively, please contact your BASF representative.
Melt Temperature 270-295 degC (518-563 degF)
Mold Temperature 80-95 degC (176-203 degF)
Injection and Packing Pressure 35-125 bar (500-1500 psi)
This product can be processed over a wide range of mold temperatures; however, for applications where aesthetics are critical, a mold surface temperature of 80-95 degC (176-203 degF) is recommended.
Injection pressure controls the filling of the part and should be applied for 90% of ram travel. Packing pressure affects the final part and can be used effectively in controlling sink marks and shrinkage. It should be applied and maintained until the gate area is completely frozen off.
Back pressure can be utilized to provide uniform melt consistency and reduce trapped air and gas. Minimal back pressure should be utilized to
prevent glass breakage.
Fast fill rates are recommended to insure uniform melt delivery to the cavity and prevent premature freezing. Surface appearance is directly affected by injection rate.
Material Data Center is provided by M-Base Engineering + Software GmbH. M-Base Engineering + Software GmbH assumes no liability for the system to be free of errors. Any decision about the application of materials must be double checked with the producer of this material.
Additional information about this material, like producer contact address, etc. can be found at www.materialdatacenter.com. For access to this extra information a registration is requested. Free online registration is available.